Starting surface speed, SFM (× 0.3048 = m/min)
Material, conditionTurning, carbideEnd mill, carbideDrill, HSSDrill, carbideTap, cut
1018, Hot rolled / annealed9754919538363
1020, Hot rolled / annealed9754919538363
1045, Annealed / normalized6844147436258
1045, Quenched & tempered6193747436258
12L14, Cold drawn5913577436258
1144, Cold drawn / stress relieved5913577436258
4140, Annealed5423287436255
4140, Quenched & tempered (pre-hard, ~28–32 HRC)3942383925155
4140, Hardened 50 HRC418——108—
4340, Annealed5423287436255
4340, Quenched & tempered3942383925155
4340, Hardened 50 HRC418——108—
8620, Annealed / as rolled7434497436255
52100, Spheroidize annealed5003027436255
52100, Hardened 60 HRC584——108—
A2, Annealed7002005824855
A2, Hardened 60 HRC584——108—
D2, Annealed7002005824855
D2, Hardened 60 HRC584——108—
H13, Annealed7002005824855
H13, Hardened & tempered (pre-hard)3681055824855
H13, Hardened 50 HRC418——108—
O1, Annealed5003027436255
O1, Hardened 60 HRC584——108—
303, Annealed5512933317630
304, Annealed5512933317630
316, Annealed5512933317630
410, Annealed6402104520230
410, Hardened & tempered3881274520230
416, Annealed6402104520230
420, Annealed6402104520230
420, Hardened & tempered3881274520230
17-4 PH, Condition A (solution annealed)4121354520230
17-4 PH, H11504481472018330
17-4 PH, H9003201052018330
2205 Duplex, Solution annealed394———30
Gray iron, Class 30, As cast9353598843648
Ductile iron, 65-45-12, As cast (ferritic/pearlitic)8533786432932
Ductile iron, 80-55-06, As cast (pearlitic)6923786432932
6061, T61,64560025065180
6061, O (annealed)1,64560025065180
7075, T6 / T6511,64560025065180
2024, T3 / T3511,64560025065180
A356 cast aluminum, T61,64560025065180
360 brass, Half hard1,31540013951372
932 bearing bronze, As cast1,31540013951372
C110 copper, Half hard—40013951372
Ti-6Al-4V, Annealed1891703912729
CP titanium, Grade 2, Annealed2831703912729
Inconel 718, Solution annealed184701511816
Inconel 718, Aged131701511816
Inconel 625, Annealed184701511816
Hastelloy X, Solution annealed184701511816