1018 steel vs 1020 steel

1020 steel carries a little more carbon (0.18–0.23 % against 0.15–0.20 %).

1018 steel and 1020 steel starting speeds by condition. 1018 steel, ISO group P: hot rolled / annealed, 975 SFM carbide turning, 491 SFM end mill. 1020 steel, ISO group P: hot rolled / annealed, 975 SFM carbide turning, 491 SFM end mill.carbide turningend millP1018 steel, Hot rolled1020 steel, Hot rolled975 SFM491 SFM
Starting speeds in SFM, the median of the makers that publish them. Bars to one scale on every material page.

Composition, side by side

Weight %. A dash means the standard sets no limit for that element.

  • 1018:

    Two published copies agree

    unless marked
  • 1020:

    Two published copies agree

    unless marked
1018 steel and 1020 steel composition, weight percent
Element10181020
C0.15–0.20 or 0.14–0.20

Published copies disagree: Chicago Tube and Summit Steel 0.15–0.20; AZoM 0.14–0.20

0.18–0.23
Mn0.60–0.90

Checked against 3 published copies

0.30–0.60
P0.04 max—
S0.05 max—

Starting cutting speeds, SFM

Same group, same starting speeds: makers give starting speeds by ISO group, not by alloy.

The calculators' starting points with no tool or setup picked. Each material page has the feeds and the makers behind them.

Starting cutting speeds in surface feet per minute
Material, conditionTurning, carbideEnd millHSS drill
1018, Hot rolled / annealedand 1020, Hot rolled / annealed97549195

Every property, sourced

1018 steel: strength, hardness and machinability

1018 steel composition

Weight %, from AISI/SAE 1018. Each limit is checked against its published copies, not averaged.

1018 steel chemical composition, weight percent
ElementLimit, %
C0.15–0.20 or 0.14–0.20

Published copies disagree: Chicago Tube and Summit Steel 0.15–0.20; AZoM 0.14–0.20

Mn0.60–0.90

Checked against 3 published copies

P0.04 max

Two published copies agree

S0.05 max

Two published copies agree

1018 steel mechanical properties

By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.

Cold drawn, typical

Tensile strength, typical
64 ksi · 441 MPa

Only two makers publish this: AZoM and Chicago Tube

Yield strength (0.2 %), typical
54 ksi · 371 MPa

Only two makers publish this: AZoM and Chicago Tube

Elongation in 2 in., typical
15 %

Only two makers publish this: AZoM and Chicago Tube

Hardness, HB
126 HB

Only two makers publish this: AZoM and Chicago Tube

Hot-rolled 1018 is weaker and more ductile; these figures are for cold-drawn bar.

Machinability ratings

Each as its publisher prints it, with the baseline it is measured against. Ratings on different baselines are not comparable, so none are averaged.

  • 70 % (AISI 1212 = 100): AZoM
  • 78 % (AISI B1112 = 100): AZoM
  • 78 % (AISI 1212 = 100): Chicago Tube
1020 steel: strength, hardness and machinability

1020 steel composition

Weight %, from AISI/SAE 1020. Each limit is checked against its published copies, not averaged.

1020 steel chemical composition, weight percent
ElementLimit, %
C0.18–0.23

Two published copies agree

Mn0.30–0.60

Two published copies agree

POnly one published copy
SOnly one published copy

1020 steel mechanical properties

By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.

Cold drawn, typical

Tensile strength, typical
Not enough published data yet
Yield strength (0.2 %), typical
Not enough published data yet
Elongation in 2 in., typical
Not enough published data yet
Hardness, HB
Not enough published data yet

Machinability ratings

Each as its publisher prints it, with the baseline it is measured against. Ratings on different baselines are not comparable, so none are averaged.

  • 65 % (AISI 1212 = 100): AZoM
Sources4