1018 steel vs 1045 steel

1045 steel carries more carbon (0.43–0.50 % against 0.15–0.20 %).

1018 steel and 1045 steel starting speeds by condition. 1018 steel, ISO group P: hot rolled / annealed, 975 SFM carbide turning, 491 SFM end mill. 1045 steel, ISO group P: annealed / normalized, 684 SFM carbide turning, 414 SFM end mill; quenched & tempered, 619 SFM carbide turning, 374 SFM end mill.carbide turningend millP1018 steel, Hot rolled975 SFM491 SFM1045 steel, Annealed684 SFM414 SFM1045 steel, Quenched & tempered619 SFM374 SFM
Starting speeds in SFM, the median of the makers that publish them. Bars to one scale on every material page.

Composition, side by side

Weight %. A dash means the standard sets no limit for that element.

  • 1018:

    Two published copies agree

    unless marked
  • 1045:

    Checked against 3 published copies

    unless marked
1018 steel and 1045 steel composition, weight percent
Element10181045
C0.15–0.20 or 0.14–0.20

Published copies disagree: Chicago Tube and Summit Steel 0.15–0.20; AZoM 0.14–0.20

0.43–0.50 or 0.42–0.50

Published copies disagree: AZoM and Chicago Tube and Summit Steel 0.43–0.50; Alro 0.42–0.50

Mn0.60–0.90

Checked against 3 published copies

0.60–0.90

Checked against 4 published copies

P0.04 max0.04 max
S0.05 max0.05 max

Starting cutting speeds, SFM

The calculators' starting points with no tool or setup picked. Each material page has the feeds and the makers behind them.

Starting cutting speeds in surface feet per minute
Material, conditionTurning, carbideEnd millHSS drill
1018, Hot rolled / annealed97549195
1045, Annealed / normalized68441474
1045, Quenched & tempered61937474

Every property, sourced

1018 steel: strength, hardness and machinability

1018 steel composition

Weight %, from AISI/SAE 1018. Each limit is checked against its published copies, not averaged.

1018 steel chemical composition, weight percent
ElementLimit, %
C0.15–0.20 or 0.14–0.20

Published copies disagree: Chicago Tube and Summit Steel 0.15–0.20; AZoM 0.14–0.20

Mn0.60–0.90

Checked against 3 published copies

P0.04 max

Two published copies agree

S0.05 max

Two published copies agree

1018 steel mechanical properties

By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.

Cold drawn, typical

Tensile strength, typical
64 ksi · 441 MPa

Only two makers publish this: AZoM and Chicago Tube

Yield strength (0.2 %), typical
54 ksi · 371 MPa

Only two makers publish this: AZoM and Chicago Tube

Elongation in 2 in., typical
15 %

Only two makers publish this: AZoM and Chicago Tube

Hardness, HB
126 HB

Only two makers publish this: AZoM and Chicago Tube

Hot-rolled 1018 is weaker and more ductile; these figures are for cold-drawn bar.

Machinability ratings

Each as its publisher prints it, with the baseline it is measured against. Ratings on different baselines are not comparable, so none are averaged.

  • 70 % (AISI 1212 = 100): AZoM
  • 78 % (AISI B1112 = 100): AZoM
  • 78 % (AISI 1212 = 100): Chicago Tube
1045 steel: strength, hardness and machinability

1045 steel composition

Weight %, from AISI/SAE 1045. Each limit is checked against its published copies, not averaged.

1045 steel chemical composition, weight percent
ElementLimit, %
C0.43–0.50 or 0.42–0.50

Published copies disagree: AZoM and Chicago Tube and Summit Steel 0.43–0.50; Alro 0.42–0.50

Mn0.60–0.90

Checked against 4 published copies

P0.04 max

Checked against 3 published copies

S0.05 max

Checked against 3 published copies

1045 steel mechanical properties

By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.

Cold drawn, typical

Tensile strength, typical
91 ksi · 627 MPa85–91 ksi

Median of 3 makers

Yield strength (0.2 %), typical
75 ksi · 517 MPa65–77 ksi

Median of 3 makers

Elongation in 2 in., typical
12 %12–16 %

Median of 3 makers

Hardness, HB
171 HB

Only two makers publish this: AZoM and Chicago Tube

Machinability ratings

Each as its publisher prints it, with the baseline it is measured against. Ratings on different baselines are not comparable, so none are averaged.

  • 57 % (AISI 1212 = 100): Chicago Tube
Sources6