17-4 PH stainless vs 316 stainless

17-4 PH stainless adds copper (3.0–5.0 %) and niobium + tantalum (0.15–0.45 %); 316 stainless adds molybdenum (2.0–3.0 %) instead.

17-4 PH stainless and 316 stainless starting speeds by condition. 17-4 PH stainless, ISO group P: Condition A (solution annealed), 412 SFM carbide turning, 135 SFM end mill; H1150, 448 SFM carbide turning, 147 SFM end mill; H900, 320 SFM carbide turning, 105 SFM end mill. 316 stainless, ISO group M: annealed, 551 SFM carbide turning, 293 SFM end mill.carbide turningend millPM17-4 PH stainless, Condition A412 SFM135 SFM17-4 PH stainless, H1150448 SFM147 SFM17-4 PH stainless, H900320 SFM105 SFM316 stainless, Annealed551 SFM293 SFM
Starting speeds in SFM, the median of the makers that publish them. Bars to one scale on every material page.

Composition, side by side

Weight %. A dash means the standard sets no limit for that element.

  • 17-4 PH:

    Checked against 3 published copies

    unless marked
  • 316:

    Two published copies agree

    unless marked
17-4 PH stainless and 316 stainless composition, weight percent
Element17-4 PH316
C0.07 max0.08 max
Mn1.0 max2.0 max
Si1.0 max0.75 max
P0.04 max0.045 max
S0.03 max0.03 max
Cr15.0–17.516.0–18.0
Ni3.0–5.010.0–14.0
Cu3.0–5.0—
Nb + Ta0.15–0.45

Two published copies agree

—
Mo—2.0–3.0
N—0.10 max

Starting cutting speeds, SFM

The calculators' starting points with no tool or setup picked. Each material page has the feeds and the makers behind them.

Starting cutting speeds in surface feet per minute
Material, conditionTurning, carbideEnd millHSS drill
17-4 PH, Condition A (solution annealed)41213545
17-4 PH, H115044814720
17-4 PH, H90032010520
316, Annealed55129333

Every property, sourced

17-4 PH stainless: strength, hardness and machinability

17-4 PH stainless composition

Weight %, from ASTM A564 (type 630). Each limit is checked against its published copies, not averaged.

17-4 PH stainless chemical composition, weight percent
ElementLimit, %
C0.07 max

Checked against 3 published copies

Mn1.0 max

Checked against 3 published copies

Si1.0 max

Checked against 3 published copies

P0.04 max

Checked against 3 published copies

S0.03 max

Checked against 3 published copies

Cr15.0–17.5

Checked against 3 published copies

Ni3.0–5.0

Checked against 3 published copies

Cu3.0–5.0

Checked against 3 published copies

Nb + Ta0.15–0.45

Two published copies agree

17-4 PH stainless mechanical properties

By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.

H900, ASTM A564, type 630 bar

Tensile strength, min
190 ksi · 1,310 MPa

Checked against 3 published copies

Yield strength (0.2 %), min
170 ksi · 1,170 MPa

Checked against 3 published copies

Elongation in 2 in., min
10 %

Checked against 3 published copies

Hardness, HRC
40 HRC min

Checked against 3 published copies

Hardness, HB
388 HB min

Two published copies agree

H1025, ASTM A564, type 630 bar

Tensile strength, min
155 ksi · 1,070 MPa

Checked against 3 published copies

Yield strength (0.2 %), min
145 ksi · 1,000 MPa

Checked against 3 published copies

Elongation in 2 in., min
12 %

Checked against 3 published copies

Hardness, HRC
35 HRC min

Checked against 3 published copies

Hardness, HB
331 HB min

Two published copies agree

H1150, ASTM A564, type 630 bar

Tensile strength, min
135 ksi · 930 MPa

Checked against 3 published copies

Yield strength (0.2 %), min
105 ksi · 725 MPa

Checked against 3 published copies

Elongation in 2 in., min
16 %

Checked against 3 published copies

Hardness, HRC
28 HRC min

Checked against 3 published copies

Hardness, HB
277 HB min

Two published copies agree

316 stainless: strength, hardness and machinability

316 stainless composition

Weight %, from ASTM A240 (type 316). Each limit is checked against its published copies, not averaged.

316 stainless chemical composition, weight percent
ElementLimit, %
C0.08 max

Two published copies agree

Mn2.0 max

Two published copies agree

Si0.75 max

Two published copies agree

P0.045 max

Two published copies agree

S0.03 max

Two published copies agree

Cr16.0–18.0

Two published copies agree

Mo2.0–3.0

Two published copies agree

Ni10.0–14.0

Two published copies agree

N0.10 max

Two published copies agree

316 stainless mechanical properties

By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.

Annealed, ASTM A240, annealed plate, sheet and strip

Tensile strength, min
75 ksi · 515 MPa

Two published copies agree

Yield strength (0.2 %), min
30 ksi · 205 MPa

Two published copies agree

Elongation in 2 in., min
40 %

Two published copies agree

Hardness, HB
217 HB max

Two published copies agree

Bar (ASTM A276) is specified similarly; cold-drawn bar is stronger.

Sources4