303 stainless vs 304 stainless
303 stainless adds sulfur (0.15 % min); 304 stainless’s specification caps it at 0.03 %.
Composition, side by side
Weight %. A dash means the standard sets no limit for that element.
- 303:
Two published copies agree
unless marked - 304:
Two published copies agree
unless marked
| Element | 303 | 304 |
|---|---|---|
| C | 0.15 max | 0.07 max or 0.08 max Published copies disagree: Atlas Steels 0.07 max; AZoM 0.08 max |
| Mn | 2.0 max | 2.0 max |
| Si | 1.0 max | 0.75 max |
| P | 0.20 max | 0.045 max |
| S | 0.15 min | 0.03 max |
| Cr | 17.0–19.0 | 17.5–19.5 or 18.0–20.0 Published copies disagree: Atlas Steels 17.5–19.5; AZoM 18.0–20.0 |
| Ni | 8.0–10.0 | 8.0–10.5 |
| N | — | 0.10 max |
Starting cutting speeds, SFM
Same group, same starting speeds: makers give starting speeds by ISO group, not by alloy.
The calculators' starting points with no tool or setup picked. Each material page has the feeds and the makers behind them.
Every property, sourced
303 stainless: strength, hardness and machinability
303 stainless composition
Weight %, from ASTM A582 (type 303). Each limit is checked against its published copies, not averaged.
| Element | Limit, % |
|---|---|
| C | 0.15 max Two published copies agree |
| Mn | 2.0 max Two published copies agree |
| Si | 1.0 max Two published copies agree |
| P | 0.20 max Two published copies agree |
| S | 0.15 min Two published copies agree |
| Cr | 17.0–19.0 Two published copies agree |
| Ni | 8.0–10.0 Two published copies agree |
303 stainless mechanical properties
By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.
Annealed bar, ASTM A582, bar
- Hardness, HB
- 262 HB max
Two published copies agree
ASTM A582 specifies only hardness for 303; tensile figures quoted elsewhere are typical, not specified.
304 stainless: strength, hardness and machinability
304 stainless composition
Weight %, from ASTM A240 (type 304). Each limit is checked against its published copies, not averaged.
| Element | Limit, % |
|---|---|
| C | 0.07 max or 0.08 max Published copies disagree: Atlas Steels 0.07 max; AZoM 0.08 max |
| Mn | 2.0 max Two published copies agree |
| Si | 0.75 max Two published copies agree |
| P | 0.045 max Two published copies agree |
| S | 0.03 max Two published copies agree |
| Cr | 17.5–19.5 or 18.0–20.0 Published copies disagree: Atlas Steels 17.5–19.5; AZoM 18.0–20.0 |
| Ni | 8.0–10.5 Two published copies agree |
| N | 0.10 max Two published copies agree |
304 stainless mechanical properties
By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.
Annealed, ASTM A240, annealed plate, sheet and strip
- Tensile strength, min
- 75 ksi · 515 MPa
Two published copies agree
- Yield strength (0.2 %), min
- 30 ksi · 205 MPa
Two published copies agree
- Elongation in 2 in., min
- 40 %
Two published copies agree
- Hardness, HB
- 201 HB max
Two published copies agree
Bar (ASTM A276) is specified similarly; cold-drawn bar is stronger.