304 stainless vs 316 stainless

316 stainless adds molybdenum (2.0–3.0 %); 304 stainless’s specification doesn’t call for it.

304 stainless and 316 stainless starting speeds by condition. 304 stainless, ISO group M: annealed, 551 SFM carbide turning, 293 SFM end mill. 316 stainless, ISO group M: annealed, 551 SFM carbide turning, 293 SFM end mill.carbide turningend millM304 stainless, Annealed316 stainless, Annealed551 SFM293 SFM
Starting speeds in SFM, the median of the makers that publish them. Bars to one scale on every material page.

Composition, side by side

Weight %. A dash means the standard sets no limit for that element.

  • 304:

    Two published copies agree

    unless marked
  • 316:

    Two published copies agree

    unless marked
304 stainless and 316 stainless composition, weight percent
Element304316
C0.07 max or 0.08 max

Published copies disagree: Atlas Steels 0.07 max; AZoM 0.08 max

0.08 max
Mn2.0 max2.0 max
Si0.75 max0.75 max
P0.045 max0.045 max
S0.03 max0.03 max
Cr17.5–19.5 or 18.0–20.0

Published copies disagree: Atlas Steels 17.5–19.5; AZoM 18.0–20.0

16.0–18.0
Ni8.0–10.510.0–14.0
N0.10 max0.10 max
Mo—2.0–3.0

Starting cutting speeds, SFM

Same group, same starting speeds: makers give starting speeds by ISO group, not by alloy.

The calculators' starting points with no tool or setup picked. Each material page has the feeds and the makers behind them.

Starting cutting speeds in surface feet per minute
Material, conditionTurning, carbideEnd millHSS drill
304, Annealedand 316, Annealed55129333

Every property, sourced

304 stainless: strength, hardness and machinability

304 stainless composition

Weight %, from ASTM A240 (type 304). Each limit is checked against its published copies, not averaged.

304 stainless chemical composition, weight percent
ElementLimit, %
C0.07 max or 0.08 max

Published copies disagree: Atlas Steels 0.07 max; AZoM 0.08 max

Mn2.0 max

Two published copies agree

Si0.75 max

Two published copies agree

P0.045 max

Two published copies agree

S0.03 max

Two published copies agree

Cr17.5–19.5 or 18.0–20.0

Published copies disagree: Atlas Steels 17.5–19.5; AZoM 18.0–20.0

Ni8.0–10.5

Two published copies agree

N0.10 max

Two published copies agree

304 stainless mechanical properties

By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.

Annealed, ASTM A240, annealed plate, sheet and strip

Tensile strength, min
75 ksi · 515 MPa

Two published copies agree

Yield strength (0.2 %), min
30 ksi · 205 MPa

Two published copies agree

Elongation in 2 in., min
40 %

Two published copies agree

Hardness, HB
201 HB max

Two published copies agree

Bar (ASTM A276) is specified similarly; cold-drawn bar is stronger.

316 stainless: strength, hardness and machinability

316 stainless composition

Weight %, from ASTM A240 (type 316). Each limit is checked against its published copies, not averaged.

316 stainless chemical composition, weight percent
ElementLimit, %
C0.08 max

Two published copies agree

Mn2.0 max

Two published copies agree

Si0.75 max

Two published copies agree

P0.045 max

Two published copies agree

S0.03 max

Two published copies agree

Cr16.0–18.0

Two published copies agree

Mo2.0–3.0

Two published copies agree

Ni10.0–14.0

Two published copies agree

N0.10 max

Two published copies agree

316 stainless mechanical properties

By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.

Annealed, ASTM A240, annealed plate, sheet and strip

Tensile strength, min
75 ksi · 515 MPa

Two published copies agree

Yield strength (0.2 %), min
30 ksi · 205 MPa

Two published copies agree

Elongation in 2 in., min
40 %

Two published copies agree

Hardness, HB
217 HB max

Two published copies agree

Bar (ASTM A276) is specified similarly; cold-drawn bar is stronger.

Sources3