4140 steel vs 1045 steel

4140 steel adds chromium (0.80–1.10 %) and molybdenum (0.15–0.25 %); 1045 steel’s specification doesn’t call for them.

4140 steel and 1045 steel starting speeds by condition. 4140 steel, ISO group P: annealed, 542 SFM carbide turning, 328 SFM end mill; quenched & tempered (pre-hard, ~28–32 HRC), 394 SFM carbide turning, 238 SFM end mill; hardened 50 HRC, none published. 1045 steel, ISO group P: annealed / normalized, 684 SFM carbide turning, 414 SFM end mill; quenched & tempered, 619 SFM carbide turning, 374 SFM end mill.carbide turningend millP4140 steel, Annealed542 SFM328 SFM4140 steel, Quenched & tempered394 SFM238 SFM1045 steel, Annealed684 SFM414 SFM1045 steel, Quenched & tempered619 SFM374 SFM
Starting speeds in SFM, the median of the makers that publish them. No published speed for 4140 steel, hardened 50 HRC. Bars to one scale on every material page.

Composition, side by side

Weight %. A dash means the standard sets no limit for that element.

  • 4140:

    Two published copies agree

    unless marked
  • 1045:

    Checked against 3 published copies

    unless marked
4140 steel and 1045 steel composition, weight percent
Element41401045
C0.38–0.430.43–0.50 or 0.42–0.50

Published copies disagree: AZoM and Chicago Tube and Summit Steel 0.43–0.50; Alro 0.42–0.50

Mn0.75–1.000.60–0.90

Checked against 4 published copies

Si0.15–0.30 or 0.15–0.35

Published copies disagree: AZoM 0.15–0.30; Chicago Tube 0.15–0.35

—
Cr0.80–1.10—
Mo0.15–0.25—
P0.035 max0.04 max
S0.04 max0.05 max

Starting cutting speeds, SFM

The calculators' starting points with no tool or setup picked. Each material page has the feeds and the makers behind them.

Starting cutting speeds in surface feet per minute
Material, conditionTurning, carbideEnd millHSS drill
4140, Annealed54232874
4140, Quenched & tempered (pre-hard, ~28–32 HRC)39423839
4140, Hardened 50 HRC418——
1045, Annealed / normalized68441474
1045, Quenched & tempered61937474

Every property, sourced

4140 steel: strength, hardness and machinability

4140 steel composition

Weight %, from AISI/SAE 4140. Each limit is checked against its published copies, not averaged.

4140 steel chemical composition, weight percent
ElementLimit, %
C0.38–0.43

Two published copies agree

Mn0.75–1.00

Two published copies agree

Si0.15–0.30 or 0.15–0.35

Published copies disagree: AZoM 0.15–0.30; Chicago Tube 0.15–0.35

Cr0.80–1.10

Two published copies agree

Mo0.15–0.25

Two published copies agree

P0.035 max

Two published copies agree

S0.04 max

Two published copies agree

4140 steel mechanical properties

By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.

Hot rolled, annealed, typical

Tensile strength, typical
Not enough published data yet
Yield strength (0.2 %), typical
Not enough published data yet
Elongation in 2 in., typical
Not enough published data yet
Hardness, HB
192 HB

Only two makers publish this: AZoM and Speedy Metals

Cold finished, annealed, typical

Tensile strength, typical
110 ksi · 755 MPa105–114 ksi

Only two makers publish this: Chicago Tube and Specialty Steel

Yield strength (0.2 %), typical
93 ksi · 639 MPa85–101 ksi

Only two makers publish this: Chicago Tube and Specialty Steel

Elongation in 2 in., typical
Not enough published data yet
Hardness, HB
211 HB

Only two makers publish this: Chicago Tube and Specialty Steel

Machinability ratings

Each as its publisher prints it, with the baseline it is measured against. Ratings on different baselines are not comparable, so none are averaged.

  • 65 % (AISI 1212 = 100, annealed): AZoM
  • 63 % (AISI B1112 = 100, hot rolled, annealed): Speedy Metals
1045 steel: strength, hardness and machinability

1045 steel composition

Weight %, from AISI/SAE 1045. Each limit is checked against its published copies, not averaged.

1045 steel chemical composition, weight percent
ElementLimit, %
C0.43–0.50 or 0.42–0.50

Published copies disagree: AZoM and Chicago Tube and Summit Steel 0.43–0.50; Alro 0.42–0.50

Mn0.60–0.90

Checked against 4 published copies

P0.04 max

Checked against 3 published copies

S0.05 max

Checked against 3 published copies

1045 steel mechanical properties

By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.

Cold drawn, typical

Tensile strength, typical
91 ksi · 627 MPa85–91 ksi

Median of 3 makers

Yield strength (0.2 %), typical
75 ksi · 517 MPa65–77 ksi

Median of 3 makers

Elongation in 2 in., typical
12 %12–16 %

Median of 3 makers

Hardness, HB
171 HB

Only two makers publish this: AZoM and Chicago Tube

Machinability ratings

Each as its publisher prints it, with the baseline it is measured against. Ratings on different baselines are not comparable, so none are averaged.

  • 57 % (AISI 1212 = 100): Chicago Tube
Sources8