6061 aluminum vs 2024 aluminum
2024 aluminum carries far more copper (3.8–4.9 % against 0.15–0.40 %).
Composition, side by side
Weight %. A dash means the standard sets no limit for that element.
- 6061:
Two published copies agree
unless marked - 2024:
Two published copies agree
unless marked
| Element | 6061 | 2024 |
|---|---|---|
| Si | 0.40–0.80 | 0.50 max |
| Fe | 0.70 max | 0.50 max |
| Cu | 0.15–0.40 | 3.8–4.9 |
| Mn | 0.15 max | 0.30–0.90 |
| Mg | 0.80–1.20 | 1.2–1.8 |
| Cr | 0.04–0.35 | 0.10 max |
| Zn | 0.25 max | 0.25 max |
| Ti | 0.15 max | 0.15 max |
Starting cutting speeds, SFM
Same group, same starting speeds: makers give starting speeds by ISO group, not by alloy.
The calculators' starting points with no tool or setup picked. Each material page has the feeds and the makers behind them.
Every property, sourced
6061 aluminum: strength, hardness and machinability
6061 aluminum composition
Weight %, from Aluminum Association (6061). Each limit is checked against its published copies, not averaged.
| Element | Limit, % |
|---|---|
| Si | 0.40–0.80 Two published copies agree |
| Fe | 0.70 max Two published copies agree |
| Cu | 0.15–0.40 Two published copies agree |
| Mn | 0.15 max Two published copies agree |
| Mg | 0.80–1.20 Two published copies agree |
| Cr | 0.04–0.35 Two published copies agree |
| Zn | 0.25 max Two published copies agree |
| Ti | 0.15 max Two published copies agree |
6061 aluminum mechanical properties
By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.
T6 / T651, Aluminum Association typical values
- Tensile strength, typical
- 45 ksi · 310 MPa
Checked against 3 published copies
- Yield strength (0.2 %), typical
- 40 ksi · 276 MPa
Checked against 3 published copies
- Elongation in 2 in., typical
- 12 %
Two published copies agree
- Hardness, HB
- 95 HB
Two published copies agree
Elongation for 1/16 in. sheet; 1/2 in. bar runs about 17 %.
O (annealed), Aluminum Association typical values
- Tensile strength, typical
- 18 ksi · 124 MPa
Two published copies agree
- Yield strength (0.2 %), typical
- 8 ksi · 55 MPa
Two published copies agree
- Elongation in 2 in., typical
- 25 %
Two published copies agree
- Hardness, HB
- Only one published copy
Machinability ratings
Each as its publisher prints it, with the baseline it is measured against. Ratings on different baselines are not comparable, so none are averaged.
- 50 % (0–100 scale of aluminum alloys, T6): ASM datasheet
2024 aluminum: strength, hardness and machinability
2024 aluminum composition
Weight %, from Aluminum Association (2024). Each limit is checked against its published copies, not averaged.
| Element | Limit, % |
|---|---|
| Si | 0.50 max Two published copies agree |
| Fe | 0.50 max Two published copies agree |
| Cu | 3.8–4.9 Two published copies agree |
| Mn | 0.30–0.90 Two published copies agree |
| Mg | 1.2–1.8 Two published copies agree |
| Cr | 0.10 max Two published copies agree |
| Zn | 0.25 max Two published copies agree |
| Ti | 0.15 max Two published copies agree |
2024 aluminum mechanical properties
By condition. Typical values vary by mill and bar size; specified minimums are what the standard guarantees.
T3, Aluminum Association typical values
- Tensile strength, typical
- 70 ksi · 483 MPa
Checked against 3 published copies
- Yield strength (0.2 %), typical
- 50 ksi · 345 MPa
Checked against 3 published copies
- Elongation in 2 in., typical
- 18 %
Two published copies agree
- Hardness, HB
- 120 HB
Two published copies agree
Elongation for 1/16 in. sheet.
Machinability ratings
Each as its publisher prints it, with the baseline it is measured against. Ratings on different baselines are not comparable, so none are averaged.
- 70 % (0–100 scale of aluminum alloys, T3): ASM datasheet
Sources4
- thyssenkrupp Materials NA, aluminum alloys (typical properties) (archived Nov 15, 2026)
- United Aluminum, 6061, 7075, 2024 composition and typical properties
- ASM material datasheet, aluminum 6061-T6 (Aluminum Association data, as reprinted) (archived Jun 10, 2026)
- ASM material datasheet, aluminum 2024-T3 (Aluminum Association data, as reprinted) (archived Aug 13, 2024)