O-ring groove chart

Gland depth and groove width (no backup ring) for each AS568 cross section. Each number is the range Parker and Apple Rubber cover between them, and each maker's own figures, with the squeeze they give, are listed under it. Gland depth is the radial distance from the groove bottom to the mating surface. The O-ring sizes are on the O-ring size chart. For the groove diameter on your own bore or rod, with the stretch and fill checked, use the O-ring groove calculator.

A 0.139" O-ring cross section in a static radial gland, in section: squeezed between the groove bottom and the bore, its free section dashed over it.free section 0.139"squeeze 14–23 %boreO-ringgland depth 0.110–0.116"groove width 0.187–0.200"piston
The .139" row as an example: the gland depth and groove width in a static radial gland. Drawn to scale at the gland’s middle depth and width.

Static radial seals (piston or rod, no motion)

Static radial seals (piston or rod, no motion): gland depth and groove width by cross section, inches
Cross sectionGland depthGroove widthEach maker
0.070"0.050–0.055"

Only two makers publish this: Parker and Apple Rubber

0.093–0.110"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.050–0.052", width 0.093–0.098", squeeze 22–32 %Apple Rubber: depth 0.050–0.055", width 0.100–0.110", squeeze 18–32 %
0.103"0.080–0.086"

Only two makers publish this: Parker and Apple Rubber

0.140–0.151"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.081–0.083", width 0.140–0.145", squeeze 17–24 %Apple Rubber: depth 0.080–0.086", width 0.141–0.151", squeeze 14–25 %
0.139"0.110–0.116"

Only two makers publish this: Parker and Apple Rubber

0.187–0.200"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.111–0.113", width 0.187–0.192", squeeze 16–23 %Apple Rubber: depth 0.110–0.116", width 0.190–0.200", squeeze 14–23 %
0.210"0.170–0.176"

Only two makers publish this: Parker and Apple Rubber

0.275–0.286"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.170–0.173", width 0.281–0.286", squeeze 15–21 %Apple Rubber: depth 0.170–0.176", width 0.275–0.285", squeeze 14–21 %
0.275"0.225–0.235"

Only two makers publish this: Parker and Apple Rubber

0.345–0.380"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.226–0.229", width 0.375–0.380", squeeze 15–20 %Apple Rubber: depth 0.225–0.235", width 0.345–0.355", squeeze 13–20 %

Face seals (axial)

Face seals (axial): gland depth and groove width by cross section, inches
Cross sectionGland depthGroove widthEach maker
0.070"0.049–0.054"

Only two makers publish this: Parker and Apple Rubber

0.100–0.110"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.050–0.054", width 0.101–0.107", squeeze 19–32 %Apple Rubber: depth 0.049–0.054", width 0.100–0.110", squeeze 19–33 %
0.103"0.074–0.081"

Only two makers publish this: Parker and Apple Rubber

0.136–0.151"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.074–0.080", width 0.136–0.142", squeeze 20–30 %Apple Rubber: depth 0.075–0.081", width 0.141–0.151", squeeze 19–29 %
0.139"0.100–0.108"

Only two makers publish this: Parker and Apple Rubber

0.177–0.200"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.101–0.107", width 0.177–0.187", squeeze 20–30 %Apple Rubber: depth 0.100–0.108", width 0.190–0.200", squeeze 20–30 %
0.210"0.152–0.165"

Only two makers publish this: Parker and Apple Rubber

0.270–0.290"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.152–0.162", width 0.270–0.290", squeeze 21–30 %Apple Rubber: depth 0.155–0.165", width 0.275–0.285", squeeze 20–28 %
0.275"0.201–0.215"

Only two makers publish this: Parker and Apple Rubber

0.342–0.362"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.201–0.211", width 0.342–0.362", squeeze 21–29 %Apple Rubber: depth 0.205–0.215", width 0.345–0.355", squeeze 20–27 %

Dynamic reciprocating seals

Dynamic reciprocating seals: gland depth and groove width by cross section, inches
Cross sectionGland depthGroove widthEach maker
0.070"0.055–0.057"

Only two makers publish this: Parker and Apple Rubber

0.090–0.100"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.055–0.057", width 0.093–0.098", squeeze 15–25 %Apple Rubber: depth 0.055–0.057", width 0.090–0.100", squeeze 15–25 %
0.103"0.087–0.090"

Only two makers publish this: Parker and Apple Rubber

0.140–0.150"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.088–0.090", width 0.140–0.145", squeeze 10–17 %Apple Rubber: depth 0.087–0.090", width 0.140–0.150", squeeze 10–18 %
0.139"0.119–0.123"

Only two makers publish this: Parker and Apple Rubber

0.180–0.192"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.121–0.123", width 0.187–0.192", squeeze 9–16 %Apple Rubber: depth 0.119–0.123", width 0.180–0.190", squeeze 9–17 %
0.210"0.183–0.188"

Only two makers publish this: Parker and Apple Rubber

0.280–0.290"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.185–0.188", width 0.281–0.286", squeeze 8–14 %Apple Rubber: depth 0.183–0.188", width 0.280–0.290", squeeze 8.5–15 %
0.275"0.234–0.240"

Only two makers publish this: Parker and Apple Rubber

0.370–0.380"

Only two makers publish this: Parker and Apple Rubber

Parker: depth 0.237–0.240", width 0.375–0.380", squeeze 11–16 %Apple Rubber: depth 0.234–0.240", width 0.370–0.380", squeeze 10.5–17 %

Sources

Apple Rubber prints one groove width ± .005"; that range is shown. Global O-Ring's inch glands follow Parker's, so they are not a separate source.