ASTM A193 · A320 · Pipe flange studs
Stud bolt grades: B7, B16, L7, B7M, B8 and B8M
The studs that bolt pipe flanges. ASTM A193 covers bolting for high-temperature or high-pressure service (B7, B16, B7M, B8, B8M), and A320 covers low-temperature service (L7). Here are the minimum strengths by diameter, the nut each grade takes, and why the B7 torque tables don't fit a stainless stud.
Minimum strength by diameter
| Grade | Diameter | Yield, ksi | Tensile, ksi | Yield, MPa |
|---|---|---|---|---|
| A193 B7 | To 2-1/2" | 105 | 125 | 724 |
| Over 2-1/2" to 4" | 95 | 115 | 655 | |
| Over 4" to 7" | 75 | 100 | 517 | |
| A193 B16 | To 2-1/2" | 105 | 125 | 724 |
| Over 2-1/2" to 4" | 95 | 110 | 655 | |
| Over 4" to 7" | 85 | 100 | 586 | |
| A320 L7 | To 2-1/2" | 105 | 125 | 724 |
| A193 B7M | To 4" | 80 | 100 | 552 |
| Over 4" to 7" | 75 | 100 | 517 | |
| A193 B8 Class 1 | All sizes | 30 | 75 | 207 |
| A193 B8M Class 1 | All sizes | 30 | 75 | 207 |
| A193 B8M Class 2 | To 3/4" | 95 | 110 | 655 |
| Over 3/4" to 1" | 80 | 100 | 552 | |
| Over 1" to 1-1/4" | 65 | 95 | 448 | |
| Over 1-1/4" to 1-1/2" | 50 | 90 | 345 |
- B7:
Checked against 3 published copies
- B16:
Two published copies agree
- L7:
Two published copies agree
- B7M:
Two published copies agree
- B8 Class 1:
Checked against 3 published copies
- B8M Class 1:
Checked against 3 published copies
- B8M Class 2:
Two published copies agree
B16 and L7 match B7's yield at every size an ASME B16.5 flange uses (to 2-1/2" for L7, the largest A320 lists). B7M is the same alloy made softer on purpose: its yield is 80 ksi to 4". Class 2 stainless is strain hardened, so its strength falls with size, and A193 lists it only to 1-1/2". MPa are converted from ksi (× 6.895), not read from the metric tables.
The nut each grade takes (ASTM A194)
B7 stud: A194 grade 2H nut
Two published copies agree
B16 stud: not shown. Only one published copy pairs a nut with this grade.
L7 stud: A194 grade 4 or 7 nut
Two published copies agree
B7M stud: not shown. Only one published copy pairs a nut with this grade.
B8 Class 1 stud: A194 grade 8 nut
Two published copies agree
B8M Class 1 stud: A194 grade 8M nut
Published copies disagree: Portland Bolt 8M; Lamons 8
B8M Class 2 stud: not shown. Only one published copy pairs a nut with this grade.
Flange studs take heavy hex nuts (ASME B18.2.2), 1-1/2 times the stud diameter plus 1/8" across the flats: a 3/4" stud's nut takes a 1-1/4" wrench.
Two published copies agree
Why B7 torque tables don't fit B8M Class 1
Show
Gasket makers' flange torque tables are written for B7 studs. Garlock's table and the 60 ksi table Lamons prints load each stud to about 60,000 psi. That is 57% of B7's 105,000 psi yield, but 2× the 30,000 psi yield of a B8 or B8M Class 1 stud. A table torque would stretch a Class 1 stainless stud past yield, so it would no longer hold its load.
For B8 or B8M Class 1, the calculator works the torque from a share of the stud's own yield (T = K × D × F) and labels it computed. Class 2 and B7M take the table scaled by their yield over B7's.
B8M Class 1 on a 4" Class 150 flange, in the calculator
From the standard, ASTM A193 minimum yield (copies above); T = K × D × F
Lubricant and nut factor (K)
K is the share of torque that becomes clamp: T = K × D × F. Less friction means a lower K, so the same torque gives more clamp.
| Condition or table | K |
|---|---|
| Plain steel, dry, as received | 0.2 |
| Oiled threads | 0.15 |
| Garlock's flange table (spiral wound) | Not printed |
| Flexitallic's flange table (spiral wound) | 0.15–0.19 |
| Teadit's flange table (spiral wound) | 0.17 |
| FNW's flange table (spiral wound) | Not printed |
| Gore's flange table (sheet) | 0.15 |
| Thomson's flange table (sheet) | 0.2 |
Dry:
Median of 4 makers
Oiled:
Median of 3 makers
Each maker's row is what that maker prints about its own table.
Copper or nickel anti-seize, moly paste and PTFE-coated studs are not listed yet: no K for them has three agreeing published sources. Use the K your lubricant's maker prints in the calculator's "My K".
Temperature ranges
Not shown: only one published table we found (Lamons) gives a service temperature range per grade, and our rule needs two. A193's scope is high-temperature or high-pressure service, and A320's is low-temperature service. Check your piping spec for the limits.
Sources15
- Lamons — Gasket Handbook 2023: fastener details (ASTM A193, A307, A320) (archived Aug 12, 2025)
- Portland Bolt — ASTM A193 and A320 specifications: mechanical properties (archived Apr 19, 2026)
- Torqbolt — ASTM A193/A193M bolting specification: mechanical property tables (archived May 14, 2026)
- Wermac — Heavy hex nuts, ASME B18.2.2, used with ASME B16.5 stud bolts (archived Jun 19, 2025)
- AMESweb — Heavy hex nut sizes and dimensions table, ASME B18.2.2 (archived Sep 16, 2025)
- Garlock — Torque tables, ASME B16.5 Class 150-2500 raised face flanges with metallic gaskets (Flexseal)
- Flexitallic — Spiral wound gasket CG and CGI torque chart, ASME B16.5
- Teadit — Suggested torque values, spiral wound 913M on ASME B16.5 raised face flanges (Nov 2010) (archived May 11, 2026)
- FNW — Torque chart: torque ratings for spiral wound gaskets, Class 150-600
- Gore — Torque guidelines: Universal Pipe Gasket and GR sheet gasketing on raised face steel flanges, ASME B16.5
- Thomson Performance Sealing — Bolt torque values, Graphite-XF sheet ring gaskets on ASME B16.5 raised face flanges (archived Nov 13, 2026)
- Fastenal — Torque-tension relationship for A307A, Grade 5, 8 and 9 bolts (Rev 3-6-09) (archived Jul 12, 2023)
- Portland Bolt — Bolt torque chart (75% of proof load) (archived Jul 22, 2026)
- AIMS Industrial — Imperial bolt torque chart (SAE J429) (archived Nov 13, 2026)
- Engineers Edge — Torque vs tension for SAE J429 bolts (archived Oct 15, 2024)