ISO 898-1 · coarse

M10 × 1.5 bolt torque

M10 × 1.5 Class 10.9: 72.2 N·m dry, 54.1 N·m lubricated, for a steel bolt tightened to 75% of its proof load.

A M10 × 1.5 Class 10.9 bolt clamping two plates, in section: the head and the nut squeeze the joint with the clamp load.clamp load 36.1 kNbolt M10 × 1.5 Class 10.9jointnut
M10 × 1.5 Class 10.9 at 75% of its proof load. Not to scale.

Tightening torque

M10 × 1.5 tightening torque by grade, dry and lubricated
GradeDry N·mLubed N·mDry ft·lbLubed ft·lbClamp load
Class 8.850.537.837.227.925.2 kN
Class 10.972.254.153.239.936.1 kN
Class 12.984.463.362.246.742.2 kN

From the standard, ISO 898-1 tensile stress area

1 ft·lb = 1.355818 N·m. Lubricated is about 75% of dry (K 0.15 vs 0.20) for the same clamp load.

What these values assume

The preload, the nut factor and the formula
  • Clamp load is 75% of the proof load of the bolt's grade (SAE J429, ISO 898-1), the usual preload for a reusable joint.
  • Dry: K = 0.20, plain steel threads as received. Lubricated: K = 0.15, oiled threads. Plated, waxed or thread-locked threads take a different K and less torque.
  • Torque T = K × D × F, D the nominal diameter, F the clamp load; tensile stress area from ASME B1.1 or ISO 898-1.
  • Steel bolt and nut (or tapped hole) at least as strong as the bolt. Tapped aluminum or cast iron needs less.

Two published copies agree

A starting value, not a spec. Torque is only an indirect measure of clamp load: thread and under-head friction decide how much of it becomes clamp. The joint designer's or equipment maker's torque wins.

Published charts

What published charts print for M10 × 1.5

Dry, on the same basis (75% of proof, K 0.20), in N·m.

Class 8.8
51.3 N·m (charts print 50.5–52.0)Only two makers publish this: Fastenal and AIMS Industrial
Class 10.9
72.1 N·m (charts print 72.0–72.2)Only two makers publish this: Fastenal and AIMS Industrial
Class 12.9
84.2 N·m (charts print 84.0–84.4)Only two makers publish this: Fastenal and AIMS Industrial

Only two makers publish this: Fastenal and AIMS Industrial

How it's worked

The arithmetic for Class 10.9

As = .7854 × (10 − .9382 × 1.5)² = 58.0 mm². Class 10.9: F = .75 × 58.0 × 830 MPa = 36,099 N; dry T = .20 × 10 mm × 36,099 N = 72.2 N·m.

Sources

Sources9