Look at a used insert before you index it: each kind of wear has its own place and cause, and the fix for one is often the opposite of another’s.

A turning insert’s corner, enlarged, from above, with wear in each place to look: a crater in the top face behind the edge, a worn flank along the edge, a notch at the depth-of-cut line and the nose pushed out of shape.insertcraterdeformed edgecutting edgeworn flanknotch
A worn insert corner, from above: where each kind of wear shows. Enlarged; not to scale.

Look before you index

A used insert is a record of the cut. Before you turn it to a fresh edge, look at the old one under a loupe or a good light, from the top and from the side. Each kind of wear sits in its own place and has its own cause, and the fix for one is often the opposite of the fix for another.

Look at the edge you actually cut with: the corner and the stretch of edge up to the depth of cut. Note where the damage is (top face, flank, the depth-of-cut line, the corner) and what it looks like (worn smooth, broken, cracked, smeared, pushed out of shape).

Flank wear is the good kind

An even, shiny land worn on the flank below the edge is normal. Every edge ends this way if nothing else gets it first, and it grows slowly and predictably, so you can plan when to index. Sandvik calls it the preferred wear type.

If it grows too fast, the edge is running too hot or the grade is too soft for the job: lower the speed, or use a more wear-resistant grade. Index before the land changes the size and the finish.

Heat and pressure: crater wear and plastic deformation

Crater wear is a hollow on the top face, a little behind the edge, where the hot chip slides over the insert. It is heat and chemistry: the chip wears the carbide away. Speed and feed come down, and a more positive geometry and a coated grade help.

Plastic deformation is the corner sagging or bulging, as the carbide goes soft from heat and load. If the edge is pushed down, lower the feed first; if it bulges out at the flank, lower the speed. A harder grade and more coolant at the edge help with both.

Notches, built-up edge, chips and cracks

Notch wear is a nick at the depth-of-cut line, where the edge meets the part’s hard skin or a work-hardened layer from the last pass. Stainless and nickel alloys are the usual cases. Vary the depth of cut between passes so the notch doesn’t land in one place, or use a round insert or a smaller entering angle.

Built-up edge is work material welded onto the edge. It tears off and takes coating with it, and it leaves a torn finish. It means the cut is too cool or the material too sticky: raise the speed, and use a sharper, more positive insert.

Chipping is small bites out of the edge, from shock, vibration, or a grade too brittle for the cut: use a tougher grade, a stronger edge and a lighter feed, and stiffen the setup. Thermal cracks are fine cracks across the edge, square to it, from the edge heating and cooling in an interrupted cut. Coolant that comes and goes causes them, so run it fully off or flood it.

Change one thing

Find the main wear type, make the one change the guides agree on, and look again after the same amount of cutting. If the wear changes type (say crater turns to flank wear), you went the right way. The troubleshooter pages list each fix with the makers who give it.

Try it on a calculator

  • Fix a turning problem — Stringy chips, chatter, a torn finish, built-up edge or chipped inserts: causes and what to change.
  • Turning speeds and feeds calculator — Material, insert and setup to speed, feed, DOC, RPM and G-code.
  • Insert grade picker — Inconel, titanium or stainless to the grade and chipbreaker a maker recommends, every maker’s equivalent, nose radius and why.

Charts

  • Tool wear chart — The seven ways an insert wears, from flank and crater wear to thermal cracks: where to look, the cause, and the fix Sandvik, Mitsubishi and Iscar give.
Check yourself: 5 questions

Check yourself

  1. 1. Which kind of wear is the normal, predictable one you want to end an edge’s life?

  2. 2. There’s a hollow on the insert’s top face, just behind the edge. What do all three wear guides change first?

  3. 3. Aluminum is welding onto the edge and the finish is torn. Which change comes first?

  4. 4. Turning stainless, the insert notches right at the depth-of-cut line. Which change spreads the wear out?

  5. 5. Facing an interrupted cut with coolant, the edge shows fine cracks across it. What do the guides say about coolant?

0 of 5 answered