Tooling & workholding · Inserts
Tool wear chart
An insert wears in seven ways: flank wear, crater wear, notch wear, built-up edge, chipping, thermal cracking and plastic deformation. Flank wear is the normal kind, and it sets tool life; each of the others points to a cause you can change. The table gives where to look and the first fix Sandvik, Mitsubishi and Iscar all give.
Insert wear types
Each drawing shows the cutting edge from the corner: the top face above it, the flank below. The wear is shaded.
| Wear | Where to look | Main cause | First fix |
|---|---|---|---|
| Flank wearAn even land on the flank, below the cutting edge | An even land on the flank, below the cutting edge | Cutting speed too high | Lower the cutting speed 3 makers agree: Sandvik · Mitsubishi · Iscar |
| Crater wearA hollow on the top face, just behind the edge | A hollow on the top face, just behind the edge | Too much heat and pressure on the top face: speed and feed too high | Lower the cutting speed and feed 3 makers agree: Sandvik · Mitsubishi · Iscar |
| Notch wearA notch at the depth-of-cut line | A notch at the depth-of-cut line | Work-hardened skin or scale at the depth-of-cut line | Use a round insert or a smaller entering angle 3 makers agree: Sandvik · Mitsubishi · Iscar |
| Built-up edgeWork material welded on top of the edge | Work material welded on top of the edge | Cutting too cool: speed too low | Raise the cutting speed 3 makers agree: Sandvik · Mitsubishi · Iscar |
| ChippingSmall bites missing along the edge | Small bites missing along the edge | A grade too hard or brittle for the cut | Use a tougher grade 3 makers agree: Sandvik · Mitsubishi · Iscar |
| Thermal crackingFine cracks across the edge, square to it | Fine cracks across the edge, square to it | The edge heating and cooling over and over: interrupted cuts, or coolant that comes and goes | Keep the coolant steady: fully off or flooded 3 makers agree: Sandvik · Mitsubishi · Iscar |
| Plastic deformationThe corner pushed down or bulged out | The corner pushed down or bulged out | Too much heat and pressure: speed and feed too high | Lower the speed and feed 3 makers agree: Sandvik · Mitsubishi · Iscar |
Each name opens its page: every cause, every fix with the makers who give it, and where they disagree.
Reading an edge
- Look at the used edge under a loupe or good light, from the top and from the side, before you index it.
- Find where the damage is: the flank, the top face, the depth-of-cut line, or the corner.
- Match it to a row above, and make the first fix only.
- Cut the same amount again and look. If the wear has turned into even flank wear, you went the right way.
Lesson: Reading tool wear ·Fix a turning problem ·Insert grades
Sources
- Sandvik Coromant — Troubleshooting in turning (archived Dec 4, 2024)
- Mitsubishi Materials — Trouble shooting for turning (archived Jul 10, 2026)
- Mitsubishi Materials — Causes of tool damage (types of cutting edge damage and solutions)
- ISCAR — ISO turn inserts wear troubleshooting
Written in our own words from each maker's guide; the drawings are ours.