Materials · Tempering
Temper color chart
On bright steel, temper colors run from pale yellow at about 428 °F (220 °C) through straw and brown to purple at 530 °F (277 °C) and blue at 550 °F (288 °C): the median of three charts. Each color is an oxide film that keeps thickening with time, so use it as a check on your temper, not as a thermometer.
Temper colors by temperature
The color a clean, bright steel surface turns when heated in air. We grouped the charts’ names by the color they describe; each chart’s own name and number is in the last column. Our swatches are approximate, and screens shift them.
| Color | Temperature | The charts call it |
|---|---|---|
| Pale yellowWest Yorkshire Steel: Light Yellow · Hinkley (1918): Pale Yellow · Colvin & Stanley (1914): faint yellow | 428 °F (220 °C)Median of 3 charts; they span 410–430 °F |
|
| StrawWest Yorkshire Steel: Straw · Colvin & Stanley (1914): straw | 430–450 °F (221–232 °C)Two charts: West Yorkshire Steel 430, Colvin & Stanley (1914) 450 |
|
| Dark strawWest Yorkshire Steel: Dark Yellow · Hinkley (1918): Golden Yellow · Colvin & Stanley (1914): dark straw | 469 °F (243 °C)Median of 3 charts; they span 460–470 °F |
|
| BrownWest Yorkshire Steel: Yellow Brown · Colvin & Stanley (1914): brown | 480–490 °F (249–254 °C)Two charts: West Yorkshire Steel 480, Colvin & Stanley (1914) 490 |
|
| PurpleWest Yorkshire Steel: Purple · Hinkley (1918): Purple · Colvin & Stanley (1914): purple | 530 °F (277 °C)Median of 3 charts; they span 520–531 °F |
|
| BlueWest Yorkshire Steel: Dark Blue · Hinkley (1918): Bright Blue · Colvin & Stanley (1914): blue | 550 °F (288 °C)Median of 3 charts; they span 550–560 °FWest Yorkshire Steel calls this “Dark Blue”; the two older charts keep that name for 600 °F. |
|
| Dark blueHinkley (1918): Dark Blue · Colvin & Stanley (1914): dark blue | 600–601 °F (316 °C)Two charts: Hinkley (1918) 601, Colvin & Stanley (1914) 600West Yorkshire Steel has lighter blues here instead (Wedgewood Blue 570 °F, Light Blue 590 °F). |
|
| Grey blueWest Yorkshire Steel: Grey Blue · Colvin & Stanley (1914): gray blue | 610 °F (321 °C)Two charts agree: West Yorkshire Steel and Colvin & Stanley (1914) |
|
Each chart as printed
| Color, as printed | °F |
|---|---|
| Light Yellow | 410 °F |
| Straw | 430 °F |
| Yellow | 450 °F |
| Dark Yellow | 460 °F |
| Yellow Brown | 480 °F |
| Red Brown | 500 °F |
| Purple | 520 °F |
| Violet | 530 °F |
| Dark Blue | 550 °F |
| Wedgewood Blue | 570 °F |
| Light Blue | 590 °F |
| Grey Blue | 610 °F |
| Grey Green | 630 °F |
| Color, as printed | °F |
|---|---|
| Pale Yellow | 428 °F |
| Golden Yellow | 469 °F |
| Purple | 531 °F |
| Bright Blue | 550 °F |
| Dark Blue | 601 °F |
| Color, as printed | °F |
|---|---|
| very faint yellow | 420 °F |
| faint yellow | 430 °F |
| light straw | 440 °F |
| straw | 450 °F |
| full straw | 460 °F |
| dark straw | 470 °F |
| old gold | 480 °F |
| brown | 490 °F |
| brown with purple spots | 510 °F |
| purple | 530 °F |
| deep purple | 550 °F |
| blue | 560 °F |
| dark blue | 600 °F |
| gray blue | 610 °F |
Why steel changes color, and why time matters
The color is not the steel itself but a thin film of iron oxide on it. As the film thickens it runs, by the National Bureau of Standards’ account, from light straw through straw, dark straw, brown and purple to dark blue and light blue. Keep heating and the colors repeat, fainter.
The film grows with time as well as heat. NBS found that a blue takes an hour or more near 500 °F but about a minute near 700 °F, and that the size and shape of the part change the time too. So a part held two hours in an oven can look darker than its temperature on the chart.
Using the colors
- Polish a spot bright and clean it. NBS found a matt or ground surface looks a little darker than a polished one, and grease, rust or a touch of the hand leaves the color uneven.
- Set the oven by a thermometer to the temperature for the hardness you need, and use the color only as a check.
- Our swatches and your screen are approximate; judge the real color in daylight.
- NBS warns the rate changes when the composition is very different, as with stainless steel, so these charts are for carbon and tool steel.
Next
- Tempering calculator: O1, A2, D2 or S7, hardness to temperature and back
- Tool steel heat treatment: hardening and the mills’ tempering charts
Sources
- West Yorkshire Steel — Steel tempering temperatures: colour chart
- Hinkley — A Few Secrets of the Metallurgist Simply Told (1918), Project Gutenberg (archived Aug 21, 2025)
- Colvin & Stanley — American Machinists’ Handbook (1914), p. 447, Internet Archive
- National Bureau of Standards — Bluing of Iron and Steel, Letter Circular LC630 (1941), govinfo (archived Jul 18, 2026)
NBS gives the order of the colors and why they form, but no temperature for each, so it is not counted in the medians. The swatches are ours.