Materials
Tempering calculator
The tempering temperature that takes a hardened tool steel to the hardness you want.
For a part already hardened as the mills say (see the O1 heat-treat page). Temper twice, at least two hours each, cooling to room temperature between.
Temper O1 for 60 HRC
480 °F (250 °C)
The mills span 475 °F–500 °F.
Median of 3 makers
- Uddeholm: 475 °F
- Böhler: 500 °F
- Industeel: 480 °F
Expect about brown on a bright spot (the charts put it near 485 °F). Color chart
About 697 HV (Brinell 654, past its recommended range), by ASTM E140.
How it works
- Each mill’s tempering curve is read back to the hardness you ask for, in a straight line between its own points, and never past its first or last point.
- Three mills give the median and their span; two give a range naming both; one alone is not shown.
- A2 and D2 harden again at a high temper (secondary hardening), so a hardness can come from a low temper or a high one. The two are worked out separately and never mixed.
- Temperatures are rounded to the nearest 5 °F (and 5 °C), as an oven is set.
- Tool steel heat treatment: hardening, the quench, and each steel’s tempering chart
- Temper color chart: the colors and why time changes them
- Hardness conversion: HRC, Brinell and Vickers
Sources
- Uddeholm Arne technical data sheet
- Böhler K460 data sheet (voestalpine)
- Industeel (ArcelorMittal) O1-2510 data sheet
- Uddeholm Rigor technical data sheet
- Böhler K305 data sheet (voestalpine)
- SIJ Metal Ravne SIHARD 2363 data sheet
- Uddeholm Sverker 21 technical data sheet
- Böhler K110 data sheet
- Industeel (ArcelorMittal) D2-2379 data sheet
- Crucible S7 data sheet DS314 (as hosted by Alpha Knife Supply)
- SIJ Metal Ravne SIHARD 2357 data sheet
- Industeel (ArcelorMittal) S7 data sheet
- West Yorkshire Steel — Steel tempering temperatures: colour chart
- Hinkley — A Few Secrets of the Metallurgist Simply Told (1918), Project Gutenberg
- Colvin & Stanley — American Machinists’ Handbook (1914), p. 447, Internet Archive
Hardness conversions are ASTM E140, as on the hardness calculator.
What next
How the tempering calculator works
O1 tempered at 400 °F (204 °C) comes out about 62 HRC, the median of three mills’ curves. Pick O1, A2, D2 or S7 and the hardness you need for the tempering temperature, or a temperature for the hardness, with each mill’s figure, the Brinell and Vickers equivalents, and the temper color to expect.