Materials · Tool steel

Tool steel heat treatment

Tempered at 400 °F (204 °C), O1 comes out about 62 HRC, A2 about 60.5, D2 about 60.5 and S7 about 57: each the median of three mills’ data sheets. Each steel’s page gives the hardening temperature the mills agree on, the quench, and the hardness at every tempering temperature from 300 to 1,200 °F.

Hardening and tempering at a glance

Tool steels: hardening temperature, quench, and hardness tempered at 400 °F
SteelHarden fromQuenchAt 400 °F
O1oil-hardening cold-work tool steel1,455–1,510 °F (790–820 °C)oil62 HRC

Median of 3 makers

A2air-hardening cold-work tool steel1,740–1,780 °F (950–970 °C)air or oil60.5 HRC

Median of 3 makers

D2high-carbon, high-chromium cold-work tool steel1,885 °F (1,030 °C)gas or oil60.5 HRC

Median of 3 makers

S7shock-resisting tool steel1,705–1,760 °F (930–960 °C), mills differair or oil57 HRC

Median of 3 makers

Not here yet: W1, 1095 and 4140. We found fewer than two mill data sheets that name each one and print its tempering data, so we don't publish a number for them.

Related tools

Hardness converter · Materials