Notch wear at the depth-of-cut line
Sandvik, Mitsubishi and Iscar all say: use a round insert or a smaller entering angle; use a more wear-resistant grade.
What you see
A notch worn into the edge right where the part’s outer skin meets it. Typical in stainless, Inconel and other work-hardening alloys.
Causes and what to change
Every fix here is from Sandvik, Mitsubishi and Iscar's troubleshooting guides, unless marked. Change one thing at a time.
Work-hardened skin or scale at the depth-of-cut line
Use a round insert or a smaller entering angle
Mitsubishi calls it a larger lead angle. The turning wizard warns about this in Inconel and stainless.
Vary the depth of cut between passes
It spreads the wear along the edge.
Only Sandvik and Iscar
Sticky, work-hardening materials
Use a more wear-resistant grade
Sandvik names an oxidation-resistant one such as cermet; Mitsubishi, a harder grade.
An edge too negative
Use a sharper edge
Only Sandvik
Where makers disagree
These point opposite ways, so they aren’t in a row above. If the changes above don’t cure it, try one side and watch.
On the corner radius
- Make it larger, and keep the depth of cut under it — Mitsubishi
- Make it smaller — Iscar
Notch wear: who gives which fix
Notch wear: which maker gives which fix
| Fix | Sandvik | Mitsubishi | Iscar |
|---|---|---|---|
| Use a round insert or a smaller entering angle | ✓ | ✓ | ✓ |
| Use a more wear-resistant grade | ✓ | ✓ | ✓ |
| Vary the depth of cut between passes | ✓ | – | ✓ |
| Use a sharper edge | ✓ | – | – |
Work it out
Often comes with
Sources
Sources4
- Sandvik Coromant — Troubleshooting in turning (archived Dec 4, 2024)
- Mitsubishi Materials — Trouble shooting for turning (archived Jul 10, 2026)
- Mitsubishi Materials — Causes of tool damage (types of cutting edge damage and solutions)
- ISCAR — ISO turn inserts wear troubleshooting
Written in our own words from each maker's troubleshooting guide.