Materials · Tool steel
O1 heat treatment
All three mills’ hardening ranges include 1,455–1,510 °F (790–820 °C). Quench it in oil, which leaves it about 64 HRC. O1 is an oil-hardening cold-work tool steel. Tempered at 400 °F (204 °C) it comes out about 62 HRC, and at 500 °F (260 °C) about 59.5 HRC: the median of three mills.
Hardening, by mill
| Mill (its data sheet) | Harden from | Quench | As quenched | Annealed |
|---|---|---|---|---|
| Uddeholm Arne (archived Oct 17, 2025) | 1,455–1,560 °F (790–850 °C) | Oil, Martempering bath | 63–65 HRC | about 190 HB |
| Böhler K460 | 1,435–1,510 °F (780–820 °C) | Oil, Salt bath | 65 HRC | about 220 HB |
| Industeel O1-2510 (archived Dec 13, 2025) | 1,435–1,510 °F (780–820 °C) | Oil, Salt bath | 64 HRC | about 212 HB |
How each mill names and charts it
- Uddeholm Arne: named on its sheet as AISI O1; tempering Hardened from 820 °C, 15 × 15 × 40 mm samples, oil, read from its tempering curve, ±0.5 HRC.
- Böhler K460: named on its sheet as O1 (AISI); tempering Hardened from 800 °C, 20 mm square, read from its tempering curve, ±0.5 HRC.
- Industeel O1-2510: named on its sheet as AISI O1; tempering Data points on its tempering curve, the data points on its curve.
Mills temper twice, cooling to room temperature between, and hold at least two hours or about an hour per inch of thickness. Hardness varies with section size and how fast the part cools.
O1 tempering chart
Hardness after hardening and tempering at each temperature. Three mills give the median and the span; two, a range naming both.
Median of 3 makers
unless marked| Temper at | Hardness |
|---|---|
| 300 °F (149 °C) | 64 HRC (63.5–64) Only two makers publish this: Böhler and Industeel |
| 350 °F (177 °C) | 63 HRC (62.5–63) Only two makers publish this: Böhler and Industeel |
| 400 °F (204 °C) | 62 HRC (span 62–62.5) |
| 450 °F (232 °C) | 60.5 HRC (span 60.5–61.5) |
| 500 °F (260 °C) | 59.5 HRC (span 59.5–60) |
| 600 °F (316 °C) | 56.5 HRC (span 56.5–57.5) |
| 700 °F (371 °C) | 53.5 HRC (span 53.5–54) |
| 800 °F (427 °C) | 50 HRC (span 50–50.5) |
| 900 °F (482 °C) | Not enough published data yet |
| 1,000 °F (538 °C) | Not enough published data yet |
| 1,100 °F (593 °C) | Not enough published data yet |
| 1,200 °F (649 °C) | Not enough published data yet |
What each mill prints at each temperature
| °F | Uddeholm | Böhler | Industeel |
|---|---|---|---|
| 300 | – | 64 | 63.5 |
| 350 | – | 63 | 62.5 |
| 400 | 62 | 62.5 | 62 |
| 450 | 60.5 | 61.5 | 60.5 |
| 500 | 59.5 | 60 | 59.5 |
| 600 | 56.5 | 57.5 | 56.5 |
| 700 | 53.5 | 54 | 53.5 |
| 800 | 50 | 50.5 | 50 |
| 900 | 46.5 | – | – |
| 1,000 | 42.5 | – | – |
| 1,100 | 37.5 | – | – |
| 1,200 | – | – | – |
Between two of a mill's own temperatures the value is interpolated in a straight line; past its first or last, nothing is shown.
Next
- Tempering calculator: the O1 temper for the hardness you need
- Temper color chart: the oxide colors from pale yellow to blue
- Hardness converter: HRC to Brinell and Vickers
- O1 material properties and cutting speeds
- Other steels: A2 · D2 · S7
Sources3
- Uddeholm Arne technical data sheet (archived Oct 17, 2025)
- Böhler K460 data sheet (voestalpine)
- Industeel (ArcelorMittal) O1-2510 data sheet (archived Dec 13, 2025)
Read 2026-11-11. A mill counts only when its own sheet names the AISI grade. Curves are read against the sheet's own gridlines.