Crater wear

Sandvik, Mitsubishi and Iscar all say: lower the cutting speed and feed; use a more open, positive geometry; use a more wear-resistant, coated grade.

What you see

A hollow worn into the insert’s top face just behind the edge, where the chip slides over it. Left to grow, it undercuts the edge until it breaks.

A hollow on the top face, just behind the edge. Top face above the edge, flank below.

Causes and what to change

Every fix here is from Sandvik, Mitsubishi and Iscar's troubleshooting guides, unless marked. Change one thing at a time.

  1. Too much heat and pressure on the top face: speed and feed too high

    • Lower the cutting speed and feed

  2. A grade without the wear resistance for the heat, often an uncoated one

    • Use a more wear-resistant, coated grade

      Mitsubishi: change an uncoated grade for a coated one.

      Also for: Chemical wear: the hot chip dissolves the carbide, worst in steel

  3. Chemical wear: the hot chip dissolves the carbide, worst in steel

    Use a more wear-resistant, coated grade — the same change as for “A grade without the wear resistance for the heat, often an uncoated one”, above.

  4. A chipbreaker too narrow for the chip

    • Use a more open, positive geometry

      A larger rake angle makes less heat.

Other changes the makers name

  • Get more coolant to the edge

    Iscar: raise the pressure and check where it points.

    Only Iscar

Crater wear: who gives which fix

Crater wear: which maker gives which fix
Which makers' wear guides give each fix for crater wear
FixSandvikMitsubishiIscar
Lower the cutting speed and feed✓✓✓
Use a more open, positive geometry✓✓✓
Use a more wear-resistant, coated grade✓✓✓
Get more coolant to the edge––✓
All seven wear types: the tool wear chart

Work it out

Often comes with

Sources

Sources4