The mills harden S7 between 1,705 and 1,760 °F (930–960 °C) and cool it in air or oil, which leaves it about 60 HRC. S7 is a shock-resisting tool steel. Tempered at 400 °F (204 °C) it comes out about 57 HRC, and at 500 °F (260 °C) about 55 HRC: the median of three mills.

Hardening, by mill

S7: each mill's hardening temperature, quench and as-quenched hardness, from its own data sheet
Mill (its data sheet)Harden fromQuenchAs quenchedAnnealed
Crucible S71,725–1,750 °F (941–954 °C)Air, Gas, Oil59–61 HRC187–220 HB
SIJ SIHARD 2357 (archived Jun 23, 2025)1,705–1,760 °F (930–960 °C)Air, Oil59–61 HRC–
Industeel S7 (archived Dec 13, 2025)1,725 °F (940 °C)Air, Oil–about 225 HB
How each mill names and charts it
  • Crucible S7: named on its sheet as S7; tempering Hardened from 1,725 °F, air cooled, its printed table.
  • SIJ SIHARD 2357: named on its sheet as AISI/SAE S7; tempering Its table of tempering temperature against hardness, its printed table.
  • Industeel S7: named on its sheet as S7; tempering Data points on its tempering curve, the data points on its curve.

Mills temper twice, cooling to room temperature between, and hold at least two hours or about an hour per inch of thickness. Hardness varies with section size and how fast the part cools.

S7 tempering chart

Hardness after hardening and tempering at each temperature. Three mills give the median and the span; two, a range naming both.

S7 tempering curve: hardness against tempering temperature from each mill's own sheet. Crucible: 400 °F 55–58, 500 °F 54–56, 600 °F 53–55, 700 °F 52–54, 800 °F 52–54, 900 °F 51–53, 1000 °F 50–52, 1100 °F 46–48, 1200 °F 40–42, 1300 °F 33–35. SIJ: 212 °F 59, 392 °F 57, 482 °F 55, 572 °F 54, 752 °F 53, 932 °F 52, 1022 °F 52, 1112 °F 48, 1202 °F 41. Industeel: 400 °F 57, 500 °F 55, 600 °F 54, 700 °F 53, 800 °F 53, 900 °F 52, 1000 °F 51, 1100 °F 47, 1200 °F 40 HRC.HRC3035404550556020040060080010001200°FCrucibleSIJIndusteel
S7: hardness against tempering temperature, one line per mill. From each mill’s own data; the table below gives every value.

Median of 3 makers

unless marked
S7: tempering temperature against hardness, HRC
Temper atHardness
300 °F (149 °C)Not enough published data yet
350 °F (177 °C)Not enough published data yet
400 °F (204 °C)57 HRC (span 55–58)
450 °F (232 °C)56 HRC (span 54.5–57)
500 °F (260 °C)55 HRC (span 54–56)
600 °F (316 °C)54 HRC (span 53–55)
700 °F (371 °C)53 HRC (span 52–54)
800 °F (427 °C)53 HRC (span 52–54)
900 °F (482 °C)52 HRC (span 51–53)
1,000 °F (538 °C)51 HRC (span 50–52)
1,100 °F (593 °C)47 HRC (span 46–48.5)
1,200 °F (649 °C)41 HRC (span 40–42)
What each mill prints at each temperature
Each mill's hardness, HRC, at each tempering temperature
°FCrucibleSIJIndusteel
300–58–
350–57.5–
40055–585757
45054.5–5755.556
50054–565555
60053–555454
70052–5453.553
80052–5452.553
90051–535252
1,00050–525251
1,10046–4848.547
1,20040–424140