Materials · Tool steel

D2 heat treatment

All three mills’ hardening ranges include 1,885 °F (1,030 °C). Quench it in gas or oil, which leaves it about 64 HRC. D2 is a high-carbon, high-chromium cold-work tool steel. Tempered at 400 °F (204 °C) it comes out about 60.5 HRC, and at 500 °F (260 °C) about 59.5 HRC: the median of three mills.

Hardening, by mill

D2: each mill's hardening temperature, quench and as-quenched hardness, from its own data sheet
Mill (its data sheet)Harden fromQuenchAs quenchedAnnealed
Uddeholm Sverker 21 (archived Nov 2, 2026)1,815–1,975 °F (990–1,080 °C)Gas, Vacuum, Martempering bath, Oil63–65 HRCabout 210 HB
Böhler K110 (archived Mar 20, 2026)1,885–1,960 °F (1,030–1,070 °C)Oil, Salt bath, Gas, Air63.5 HRCabout 250 HB
Industeel D2-2379 (archived Dec 13, 2025)1,885 °F (1,030 °C)Gas, Oil–about 250 HB
How each mill names and charts it
  • Uddeholm Sverker 21: named on its sheet as AISI D2; tempering Hardened from 1,020 °C, 15 × 15 × 40 mm samples, forced air, read from its tempering curve, ±0.5 HRC.
  • Böhler K110: named on its sheet as D2 (AISI); tempering Hardened from 1,070 °C, read from its tempering curve, ±0.5 HRC.
  • Industeel D2-2379: named on its sheet as AISI D2; tempering Hardened from 1,050 °C, 80 mm plate, oil, read from its tempering curve, ±0.5 HRC.

Mills temper twice, cooling to room temperature between, and hold at least two hours or about an hour per inch of thickness. Hardness varies with section size and how fast the part cools.

D2 tempering chart

Hardness after hardening and tempering at each temperature. Three mills give the median and the span; two, a range naming both.

D2 tempering curve: hardness against tempering temperature from each mill's own sheet. Uddeholm: 400 °F 60.5, 450 °F 60, 500 °F 59.5, 550 °F 59, 600 °F 59, 650 °F 59, 700 °F 59, 750 °F 59, 800 °F 59.5, 850 °F 59.5, 900 °F 60, 950 °F 59, 1000 °F 55.5, 1050 °F 50.5, 1100 °F 46. Böhler: 200 °F 61.5, 250 °F 61, 300 °F 60, 350 °F 59.5, 400 °F 59, 450 °F 58.5, 500 °F 58, 550 °F 58, 600 °F 57.5, 650 °F 57.5, 700 °F 58, 750 °F 58, 800 °F 58, 850 °F 58.5, 900 °F 60.5, 950 °F 62, 1000 °F 60.5, 1050 °F 55. Industeel: 250 °F 64.5, 300 °F 64, 350 °F 63, 400 °F 62.5, 450 °F 62, 500 °F 61, 550 °F 60.5, 600 °F 60, 650 °F 59.5, 700 °F 59, 750 °F 59, 800 °F 59, 850 °F 59.5, 900 °F 60, 950 °F 60.5, 1000 °F 60.5, 1050 °F 59, 1100 °F 56 HRC.HRC45505560652004006008001000°FUddeholmBöhlerIndusteel
D2: hardness against tempering temperature, one line per mill. From each mill’s own data; the table below gives every value.

Median of 3 makers

unless marked
D2: tempering temperature against hardness, HRC
Temper atHardness
300 °F (149 °C)62 HRC (60–64)

Only two makers publish this: Böhler and Industeel

350 °F (177 °C)61.5 HRC (59.5–63)

Only two makers publish this: Böhler and Industeel

400 °F (204 °C)60.5 HRC (span 59–62.5)
450 °F (232 °C)60 HRC (span 58.5–62)
500 °F (260 °C)59.5 HRC (span 58–61)
600 °F (316 °C)59 HRC (span 57.5–60)
700 °F (371 °C)59 HRC (span 58–59)
800 °F (427 °C)59 HRC (span 58–59.5)
900 °F (482 °C)60 HRC (span 60–60.5)
1,000 °F (538 °C)60.5 HRC (span 55.5–60.5)
1,100 °F (593 °C)51 HRC (46–56)

Only two makers publish this: Uddeholm and Industeel

1,200 °F (649 °C)Not enough published data yet
What each mill prints at each temperature
Each mill's hardness, HRC, at each tempering temperature
°FUddeholmBöhlerIndusteel
300–6064
350–59.563
40060.55962.5
4506058.562
50059.55861
6005957.560
700595859
80059.55859
9006060.560
1,00055.560.560.5
1,10046–56
1,200–––

Between two of a mill's own temperatures the value is interpolated in a straight line; past its first or last, nothing is shown.

Next

Sources3

Read 2026-11-11. A mill counts only when its own sheet names the AISI grade. Curves are read against the sheet's own gridlines.