Materials · Tool steel

A2 heat treatment

All three mills’ hardening ranges include 1,740–1,780 °F (950–970 °C). Cool it in air or oil, which leaves it about 63.5 HRC. A2 is an air-hardening cold-work tool steel. Tempered at 400 °F (204 °C) it comes out about 60.5 HRC, and at 500 °F (260 °C) about 58.5 HRC: the median of three mills.

Hardening, by mill

A2: each mill's hardening temperature, quench and as-quenched hardness, from its own data sheet
Mill (its data sheet)Harden fromQuenchAs quenchedAnnealed
Uddeholm Rigor (archived Jul 20, 2025)1,695–1,780 °F (925–970 °C)Air, Gas, Vacuum, Martempering bath, Oil63–64 HRCabout 215 HB
Böhler K3051,740–1,795 °F (950–980 °C)Oil, Salt bath, Gas, Air65 HRCabout 240 HB
SIJ SIHARD 2363 (archived Nov 13, 2026)1,705–1,780 °F (930–970 °C)Air, Oil, Salt bath63 HRC–
How each mill names and charts it
  • Uddeholm Rigor: named on its sheet as AISI A2; tempering Hardened from 925 °C, small samples, read from its tempering curve, ±0.5 HRC.
  • Böhler K305: named on its sheet as A2 (AISI); tempering Hardened from 970 °C, 20 mm square, oil, read from its tempering curve, ±0.5 HRC.
  • SIJ SIHARD 2363: named on its sheet as AISI/SAE A2; tempering Its table of tempering temperature against hardness, its printed table.

Mills temper twice, cooling to room temperature between, and hold at least two hours or about an hour per inch of thickness. Hardness varies with section size and how fast the part cools.

A2 tempering chart

Hardness after hardening and tempering at each temperature. Three mills give the median and the span; two, a range naming both.

A2 tempering curve: hardness against tempering temperature from each mill's own sheet. Uddeholm: 400 °F 60, 450 °F 59, 500 °F 58.5, 550 °F 57.5, 600 °F 57, 650 °F 56.5, 700 °F 56.5, 750 °F 56, 800 °F 56, 850 °F 55.5, 900 °F 55.5, 950 °F 55, 1000 °F 53, 1050 °F 49.5, 1100 °F 45.5, 1150 °F 41, 1200 °F 36. Böhler: 200 °F 64, 250 °F 63, 300 °F 62.5, 350 °F 61.5, 400 °F 60.5, 450 °F 59.5, 500 °F 58.5, 550 °F 58, 600 °F 58, 650 °F 57.5, 700 °F 57.5, 750 °F 57.5, 800 °F 57.5, 850 °F 57.5, 900 °F 58, 950 °F 58, 1000 °F 57, 1050 °F 55.5, 1100 °F 52.5. SIJ: 212 °F 63, 392 °F 62, 572 °F 58, 752 °F 57, 932 °F 57, 1112 °F 51, 1292 °F 36 HRC.HRC3540455055606520040060080010001200°FUddeholmBöhlerSIJ
A2: hardness against tempering temperature, one line per mill. From each mill’s own data; the table below gives every value.

Median of 3 makers

unless marked
A2: tempering temperature against hardness, HRC
Temper atHardness
300 °F (149 °C)62.5 HRC (62.5–62.5)

Only two makers publish this: Böhler and SIJ

350 °F (177 °C)62 HRC (61.5–62)

Only two makers publish this: Böhler and SIJ

400 °F (204 °C)60.5 HRC (span 60–62)
450 °F (232 °C)59.5 HRC (span 59–60.5)
500 °F (260 °C)58.5 HRC (span 58.5–59.5)
600 °F (316 °C)58 HRC (span 57–58)
700 °F (371 °C)57.5 HRC (span 56.5–57.5)
800 °F (427 °C)57 HRC (span 56–57.5)
900 °F (482 °C)57 HRC (span 55.5–58)
1,000 °F (538 °C)54.5 HRC (span 53–57)
1,100 °F (593 °C)51.5 HRC (span 45.5–52.5)
1,200 °F (649 °C)40 HRC (36–43.5)

Only two makers publish this: Uddeholm and SIJ

What each mill prints at each temperature
Each mill's hardness, HRC, at each tempering temperature
°FUddeholmBöhlerSIJ
300–62.562.5
350–61.562
4006060.562
4505959.560.5
50058.558.559.5
600575858
70056.557.557.5
8005657.557
90055.55857
1,000535754.5
1,10045.552.551.5
1,20036–43.5

Between two of a mill's own temperatures the value is interpolated in a straight line; past its first or last, nothing is shown.

Next

Sources3

Read 2026-11-11. A mill counts only when its own sheet names the AISI grade. Curves are read against the sheet's own gridlines.